              GB5310 standard 12Cr1MoV high alloy seamless steel pipe 
               bearing capacity parameters allowable stress lookup table
                            Chemical composition of high-pressure alloy steel pipe
  
  steel  
           Chemical composition(%)
       C
        Si
       Mn
      P
     S
       Cr
      Mo
         V
12Cr1MoV 
0.08~0.15
 0.17~0.37
 0.40~0.70
 ≤0.035
 ≤0.035
 0.90~1.20
 0.25~0.35
  0.15~0.30
                      
                         Mechanical properties of alloy seamless steel pipe

steel
WT(mm)
 бb(Mpa)
 бs(Mpa)
 δ5(%)
  aku(J)


12Cr1MoV
   ≤16
470~640
    ≥255
   ≥21
    ≥59



                          Alloy seamless steel pipe allowable stress
steel
WT(mm)
Allowable stress (Mpa) under the following temperature (℃)
≤20
100
200
300
350
400
500
525
550
575
12Cr1MoV
≤16
147
144
126
110
104
98
89
82
57
35